Potassium Dihydrogen Phosphate (KDP) and Potassium Dideuterium Phosphate (KD*P ) are among the most widely-used commercial NLO materials. They are commonly used for doubling, tripling and quadrupling of Nd:YAG laser at the room temperature. In addition, they are also excellent electro-optic crystals with high electro-optic coefficients, widely used as electro-optical modulators, Q-switches, and Pockels Cells, etc.

 

 

Good UV transmission

High optical damage threshold

High birefringence High nonlinear coefficients

Physical and Optical Properties:

KDP

KD*P(DKDP)

Chemical Formula

KH2PO4

KD2PO4

Crystal Structure

Tetragonal

Tetragonal

Transmission Range

200-1500nm

200-1600nm

Nonlinear Coefficients

d36=0.44pm/V

d36=0.40pm/V

Refractive Indcies
(at 1064nm)
no=1.4938,ne=1.4599

no=1.4948, ne=1.4554

Electro-Optical Coefficients

r41=8.8pm/V
r
63=10.3pm/V

r41=8.8pm/V
r
63=25pm/V

Longitudinal Half-Wave Voltage

Vp=7.65KV(l=546nm)

Vp=2.98KV(l=546nm)

Absorption

0.07/cm

0.006/cm

Temperature Synchronism Width

11.5 oC*cm

7.4 oC*cm

Spectral Synchronism Width

106 Å*cm

32 Å*cm

Angle Synchronism Width

0.84 mrad*cm

0.94 mrad*cm

Absorption Coefficient, cm-1

0.07

0.006

Mohs Hardness

2.5

2.5

Optical Damage Threshold

>5 GW/cm2

>3 GW/cm2

Extinction Ratio

30dB

Sellmeier Equations
KDP no2 = 2.259276 + 0.01008956/(l2 - 0.012942625) + 13.005522l2/(l2 - 400)
ne2 = 2.132668 + 0.008637494/(
l2 - 0.012281043) + 3.2279924l2/(l2 - 400)
DK*P no2 = 1.9575544 + 0.2901391/(l2 - 0.0281399) - 0.02824391l2 +0.004977826l4
ne2 = 1.5005779 + 0.6276034/(l2 - 0.0131558) - 0.01054063l2 +0.002243821l4

Application:
  Second, third, and fourth harmonic generation of Nd:lasers.

Frequency doubling of dyer laser

High power laser frequency conversion materials

Shutter for high speed photography

Electro-optical modulator and Q switches

KD*P Single Crystals — Standard

Designation

Operation

Input

Output

53.7 °

SHG (II)

1064 nm

532 nm

59.5°

THG (II)

1064 nm + 532 nm

355 nm

63.7°

SFM (II)

1064 nm + (421-1000 nm)

302-515 nm

86°

FHG (I) angle tune

532 nm

266nm

90°

FHG (I) temp. tune

532 nm

266 nm

36.6°

SHG (I)

1064 nm

532 nm

46.8°

THG(I)

1064 nm + 532 nm

355 nm

KD*P Specifications

Wavefront distortion:

less than l/8 @ 633nm

Dimension tolerance:

(W± 0.1mm) x (H±0.1mm) x (L + 0.2mm/-0.1mm)

Clear aperture:

> 90% central area

Flatness:

l/8 @ 633nm

Scratch/Dig code:

10/5 to MIL-O-13830A

Parallelism:

better than 20 arc seconds

P erpendicularity:

5 arc minutes

Angle tolerance:

Dq <± 0.3°, Df <±0.3°

Quality Warranty Period:

one year under proper use

Note:

1. KDP, KD*P&LiIO3   is highly hygroscopic and the coating can not be available. Please keep it in a dry environment, and sealed housing is recommended.

2.The LiIO3 crystals is available too.

3.KD*P & KDP are among the most widely-used commercial NLO materials, characterized by good UV transmission, high damage threshold, and high birefringence, though their NLO coefficients are relatively low.Because their polished surfaces are easy subject to moisten, the user recommends a dry condition (<50%) and the sealed housing for preservation.

Note: The LiIO3 crystals is available too.



 